Corrosion protection – knowledge that can save a fortune
Corrosion costs ship operators enormous sums every year. On ships it is worst below the waterline and therefore hard to see except in dry dock. Vessels often come out of the water with their anodes partly or fully consumed, a corroded propeller and sometimes corroded welds. Propeller repairs are very expensive, and so is replacing hull plates and welds. As owners keep vessels at sea for longer, effective corrosion protection matters more than ever. With modern technology, steel below the waterline can be almost fully protected.
There are two basic approaches: keeping water and oxygen away with coatings, and applying an electrical current to the metal to slow the corrosion process (cathodic protection). Experience shows that combining both gives the best and most economical result.
What determines anode life?
Owners often wonder why hull anodes last for different lengths of time. The vessel is fitted with as many anodes as ever, yet comes up with no anode left and damaged hull and propeller. Stray currents are a known cause, but other factors matter too, such as unusual coating loss.
Protecting steel in seawater requires a certain current per square metre. Demand depends on coating condition and water velocity, i.e. vessel speed. Anode life therefore depends largely on the coating and the operating conditions. The propeller moves through the water fastest and is uncoated, so it needs the most current.
How many anodes?
Typically 15–30 mA per m² of underwater area is used for a well-coated hull, whereas bare steel needs 100–300 mA/m². If a hull is painted in poor conditions and the coating adheres badly, anodes may be consumed much faster than normal.
Anodes behave like batteries delivering current in proportion to their size. A common 3.2 kg aluminium anode (2.6 kg net) delivers up to 500 mA. Aluminium anode material holds about 2,700 Ah per kg, so this anode can deliver 0.5 A for about 19 months under normal conditions. Aluminium anodes form an oxide film that limits their output, so generous numbers can safely be fitted; up to 60 mA/m² is common on Icelandic trawlers to reach up to two years' life. Anode size should match the intended life: many small anodes give more current than fewer large ones of the same weight, and are consumed sooner. Too many zinc anodes, however, can cause over-protection, coating disbondment and corrosion.
Seawater tanks
Seawater tanks also need protection. Demand is lower than on the outer hull but can still be significant if tanks are poorly protected, so anodes should be fitted in all seawater tanks and checked at every docking.
Corrosion can be measured
Simple instruments show how effective hull protection is. A small reference electrode is lowered into the water alongside and the potential between it and the hull is measured with an accurate voltmeter. There is no need for uncertainty about whether protection is working.
Why do propellers corrode?
A propeller may need up to 1,000 mA/m², and its life depends heavily on how well it is protected. That in turn depends entirely on the electrical connection between shaft and hull. The shaft runs on an oil film in its bearings, so the connection is often poor, especially once bearings are run in. A corroded propeller can therefore be a sign of good bearings!
What can be done?
The key is to keep the propeller permanently bonded to the hull. The best solution is a shaft slip ring with a thick silver track and silver/graphite brushes. Ordinary carbon brushes on the bare shaft have too much resistance. Without a slip ring, 200–300 mV between hull and propeller is common; a poor slip ring brings it to 100–250 mV; a silver slip ring with silver/graphite brushes brings it down to about 10 mV.
Cavitation and corrosion
Propeller damage is often blamed entirely on cavitation, as if nothing could be done. Experience shows that adequate cathodic protection of the propeller, from anodes or ICCP, can significantly reduce combined cavitation-corrosion damage.
Safety and service life
Anodes have a limited life, so monitoring them is essential. Over time they waste away and their output falls, while protection demand rises as the coating deteriorates. Anodes of the wrong alloy may not work at all and give false security. Regular measurement and topping up anodes as needed can cut maintenance costs significantly.
Impressed current cathodic protection
The most advanced option is ICCP, where demand is measured continuously and current is controlled accordingly. The system comprises a controller with power supply, anodes, reference electrodes and a slip ring, with alarms if protection drifts outside set limits. Many Icelandic vessels use such systems, including Dettifoss with Cathelco ICCP. More about ICCP →
Marine growth and corrosion protection for seawater systems
Mussel and marine growth in seawater pipework can be prevented and corrosion greatly reduced with copper and aluminium anodes in sea inlets or strainers, controlled by a panel. More about MGPS →
The author is managing director of Stálvélar ehf., which specialises in corrosion and marine growth protection for ships.